                                                            Product Description and Application 產品描述和用途
                                                            EHH is a kind of jacketing compounds with high-density polyethylene as the basic raw material, and mainly used for the jacketing of fibre optical cables and submarine power cables. The highest working temperature is 80℃.
                                                            EHM70 is a kind of jacketing compounds with medium-density polyethylene as the basic raw material, and mainly used for the jacketing of communication cables, control cables, signal cables and fibre optical cables. The highest working temperature is 70℃.
                                                            EHL70 is a kind of jacketing compounds with low-density polyethylene as the basic raw material, and mainly used for the jacketing of communication cables which is environmental stress cracking resistant, control cables, signal cables and power cables. The highest working temperature is 70℃.
                                                            EHH是以高密度聚乙烯為主要基材的電纜護層級材料,主要用于光纜和海底電力電纜的護層,最高工作溫度80℃。
                                                            EHM70是以中密度聚乙烯為主要基材的電纜用護層級材料,主要用于通信電纜、控制電纜、信號電纜和光纜的護層,最高工作溫度70℃。
                                                            EHL70是以線性低密度聚乙烯為基材的電纜用護層級材料,主要用于耐環境開裂的通信電纜、控制電纜、信號電纜和電力電纜的護層,最高工作溫度70℃。
                                                             
                                                             
                                                             
                                                             
                                                            Processing Indicator 加工工藝
                                                            Recommend to process with the PE extruder with L/D is more than 25.
                                                            建議使用長徑比大于25的聚乙烯用擠出機進行加工。
                                                            Model
                                                            牌號
                                                            Machine Barrel Temperature
                                                            機筒溫度
                                                            Molding Temprature
                                                            機頭溫度
                                                            EHH 150-220℃ 220-230℃
                                                            EHL 130-200℃ 190-210℃
                                                            EHM 150-220℃ 220-230℃
                                                             
                                                             
                                                            Physical and Electrical Properties 物理和電氣性能
                                                            Item
                                                            試驗項目
                                                            Unit
                                                            單位
                                                            Technical requirements
                                                            技術要求
                                                            EHH EHL EHM
                                                            Density
                                                            密度
                                                            g/cm3 0.950~0.978 0.940~0.960 0.920~0.945
                                                            熔融指數 g/10min ≤0.5 ≤0.85 ≤2.0
                                                            Tensile Strength
                                                            拉伸強度
                                                            MPa ≥20.0 ≥20.0 ≥14.0
                                                            Elongation at Break
                                                            斷裂伸長率
                                                            % ≥650 ≥650 ≥700
                                                            Brittle Temperature with Low Temperature
                                                            低溫脆化溫度
                                                            °C ≤-76 ≤-76 ≤-76
                                                            Vicat Softening Point
                                                            維卡軟化點
                                                            °C ≥110 ---- ----
                                                            Resistance to environmental stress cracking F0
                                                            耐環境應力開裂F0
                                                            h ≥500 ≥500 ≥500
                                                            20℃Volume Resistivity
                                                            20℃體積電阻率
                                                            Ω·m ≥1.0×1014 ≥1.0×1014 ≥1.0×1014
                                                            20℃Dielectric Strength,50Hz
                                                            20℃介電強度, 50Hz
                                                            MV/m ≥25.0 ≥25.0 ≥25.0
                                                            20℃Dielectric Constant,50Hz
                                                            20℃介電常數, 50Hz
                                                            / ≤2.80 ≤2.75 ≤2.80
                                                            Carbon Black Dispersion
                                                             
                                                            碳黑分散性
                                                            Carbon Black Dispersion
                                                            碳黑分散度
                                                            / ≥6 ≥6 ≥6
                                                            Absorption Coefficient
                                                            吸收系數
                                                            / ≥400 ≥400 ≥400
                                                            Carbon Black Content
                                                            碳黑含量
                                                            % 2.60±0.25 2.60±0.25 2.60±0.25
                                                            200 ℃Oxidation Induction Time
                                                             200℃氧化誘導期
                                                            min ≥30 ≥30 ≥30
                                                             
                                                             